Shop Reference for Students and Apprentices, Second Edition

Materials

Nominal Composition and Properties of Everdur

Table 17: Nominal Composition and Properties of Everdur

Desig. No.

Nominal Composition [a]

Temper [b]

Strength, Thousands of Pounds per Square Inch

Percent Elongation

Cu

Si

Mn

Pb

Al

Tensile

Yield

A

52

15

35 c

HRA

50

18

40

CRA

52

18

35

1010

95.80

3.10

1.10

CRHH

71

40

10

CRH

70 to 85

60

3

H

38 to 50

17 to 8 [c]

1015

98.25

1.50

0.25

AP

38

10

35

HP

50

40

8 to 6 [c]

XHB

75 to 85

45 to 55

1012

95.60

3.00

5.00

0.40

A

52

15

35 [c]

H

85

50

13 to 8 [c]

1000

94.90

4.00

1.10

AC

45

15

1014

90.75

2.00

7.25

A

75 to 90

37.5 to 45

12 to 9 [c]

Designation numbers are those of The American Brass Co.

The values given for the tensile strength, yield strength and elongation are all minimum values. Where ranges are shown, the first values given are for the largest diameter or largest size specimens. Yield strength values were determined at 0.50 per cent elongation under load.

[a]The following chemical symbols...

UNLIMITED FREE
ACCESS
TO THE WORLD'S BEST IDEAS

SUBMIT
Already a GlobalSpec user? Log in.

This is embarrasing...

An error occurred while processing the form. Please try again in a few minutes.